Synthetic Albany Slip Recipes
Ceramics Monthly, October 1988, Pg 49: Synthetic Albany Slip by Gerald Rowan.
Synthetic Albany Slip 1:
Dolomite 8.5%
Pearl Ash 4.0%
Soda Ash 1.0%
Unwashed Softwood Ash 10.5%
Kentucky Ball Clay (OM-4) 50%
Flint 20.0%
Red Iron Oxide 6%
Total: 100.0%
Synthetic Albany Slip 2:
Dolomite 9%
Soda Ash 1%
Cedar Heights Redart Clay 90%
Total: 100%
Synthetic Albany Slip 3:
Dolomite 9%
Soda Ash 1%
Terra Sigillata made from Cedar Heights Redart 90%
Total: 100%
Synthetic Albany Slip (Tony Hansen):
Talc 7%
Whiting 9.5%
Nepheline Syenite 14%
Redearth Clay 67.5%
Black Iron Oxide 2.0%
Total: 100%
_ Redearth clay from IMC in Medicine Hat, Alberta_
Albany slip sub. Lili Krakowski
via Alisa Liskin Clausen
58 Redart
8 Dolomite
25 Whiting